I put a coat on the underside/no show surfaces today.
All surfaces primed with 2 coats Zinsser BIN, lightly sanded with 320
SW Pro Classic acrylic satin
thinned ~5% with water (1.5 oz in 1 qt paint)
added ~3% GF Extender (1 oz in 1 qt paint)
Rolled on with a foam roller.
The paint dried pretty quick, ~20 minutes, some areas looked to be dry sooner.
Temp was 70F and the Relative Humidity was ~35%
Results look decent to me, but I have no past experience for comparison.
I can see a slight texture from the roller.
My guess is I could add another 5% Extender, especially with the low RH…?